Bitumen 90/10 is a highly specialized grade of oxidized bitumen, characterized by its exceptional hardness, high melting point, and low penetration value. With a softening point of approximately 90°C and a penetration value of 10 dmm (tenths of a millimeter), it is primarily used in industrial applications that demand rigidity, chemical resistance, and stability under extreme conditions. This grade is a semi-solid material with excellent adhesive and waterproofing properties, making it suitable for environments where strength and durability are critical.
Bitumen 90/10 is widely utilized in the production of electrical insulation materials, anti-corrosion coatings for pipes, adhesives, and sealing compounds. Its low penetration value and high softening point ensure resistance to deformation and melting under heat, making it ideal for hot climates or applications exposed to high temperatures. Additionally, it provides superior protection against moisture and chemicals, making it effective in waterproofing and protective coatings for industrial infrastructure. Manufactured through a controlled oxidation process to meet international quality standards, Bitumen 90/10 delivers consistent performance and long-lasting reliability, making it an indispensable material for demanding industrial and construction needs.
Bitumen 85/100 |
Characteristics |
Unit |
Specification |
Test Method |
Penetration @ 25 °C |
0.1 mm |
60-70 |
ASTM D-5 |
Specific gravity @ 25 °C |
gr/cm3 |
1.01-1.060 |
ASTM D-70 |
Softening Point |
°C |
46-56 |
ASTM D-36 |
Ductility @ 25 °C |
Cm |
100 Min |
ASTM D-113 |
Loss on heating |
% wt |
0.2 Max |
ASTM D-6 |
Drop in penetration after heating |
% |
20 Max |
ASTM D-6 & D-5 |
Flash Point |
°C |
250 Min |
ASTM D-92 |
Solubility in CS2 |
% wt |
99.0 Min |
ASTM D-4 |
Organic matter insoluble in CS2 |
% wt |
0.2 Max |
ASTM D-4 |
Viscosity @ 60 °C |
p |
2000±400 |
ASTM D-2171 |
Spot test |
– |
Negative |
*A.A.S.H.O.T.102 |
Different bitumen penetration Grades |
Characteristics |
Unit |
30/40 |
50/70 |
100/120 |
160/220 |
200/300 |
Test Method |
Specific gravity @ 25 °C |
gr/cm3 |
1.01-1.06 |
1.01-1.06 |
1.01-1.04 |
1.01-1.06 |
1.01±0.05 |
ASTM D-70 |
Penetration @ 25 °C |
0.1 mm |
30-40 |
50-70 |
100-120 |
160-220 |
200-300 |
ASTM D-5 |
Softening Point (R &B) |
°C |
55-63 |
46-54 |
42-49 |
35-43 |
34-41 |
ASTM D-36 |
Softening Point (R &B) |
°C |
55-63 |
46-54 |
42-49 |
35-43 |
34-41 |
ASTM D-36 |
Ductility @ 25 °C |
Cm |
100 |
100 |
100 |
100 |
100 |
ASTM D-113 |
Loss on heating, Max |
% wt |
0.2 |
0.2 |
0.2 |
0.2 |
1.3 |
ASTM D-6 |
Drop in Penetration after heating, Max |
% |
20 |
20 |
20 |
20 |
- |
ASTM D-6 & D-5 |
Flash Point. Min |
°C |
250 |
230 |
250 |
220 |
177 |
ASTM D-92 |
Solubility in CS2 |
% wt |
99.5 |
99 |
99.5 |
99 |
99 |
ASTM D-4 |
Spot test |
- |
Negative |
Negative |
Negative |
Negative |
Negative |
*A.A.S.H.O.T.102 |
Oxidized Bitumen |
Characteristics |
Unit |
85/25 |
95/25 |
90/15 |
9115/15 |
Test Method |
Penetration @ 25°C, 100 gm, 5 Seconds |
0.1 mm |
20/30 |
25/30 |
10/20 |
10/20 |
ASTM D-5 |
Specific gravity @25°C |
gr/cm³ |
1.01/1.05 |
1.01/1.05 |
1.01/1.05 |
1.01/1.05 |
ASTM D-70 |
Softening Point (R&B) |
°C |
80/90 |
90/100 |
85/95 |
110/120 |
ASTM D-36 |
Loss on heating, Max |
% wt |
0.2 |
0.2 |
0.2 Max |
0.2 |
0.2 |
Flash Point (Cleveland Open Cup), Min |
°C |
260 |
260 |
225 |
260 |
ASTM D 92 |
Performance Grades Bitumen (PG) |
High Temperature Performance |
Low Temperature Performance |
PG 46 |
-46, -40, -34 |
PG 52 |
-46, -40, -34, -28, -22, -16, -10 |
PG 58 |
-40, -34, -28, -22, -16, -10 |
PG 64 |
-40, -34, -28, -22, -16, -10 |
PG 70 |
-40, -34, -28, -22, -16, -10 |
PG 76 |
-34, -28, -22, -16, -10 |
PG 82 |
-34, -28, -22, -16, -10 |
Viscosity Grades Bitumen (VG) |
Characteristics |
Unit |
VG 40 |
VG 30 |
VG 20 |
VG 10 |
Test Method |
Absolute Viscosity @ 60°C, Poises |
°C |
Min. 2200 |
Min. 2400 |
Min. 1600 |
Min. 800 |
IS 1206 (Part 2) |
Kinematic Viscosity @ 135°C |
cSt |
Min. 400 |
Min. 350 |
Min. 300 |
Min. 250 |
IS 1206 (Part 3) |
Softening Point (R&B) |
°C |
Min. 50 |
Min. 47 |
Min. 45 |
Min. 40 |
IS 1205 |
Flash Point (Cleveland Open Cup) |
°C |
Min. 220 |
Min. 220 |
Min. 220 |
Min. 220 |
IS 1209 |
Solubility in trichloroethylene |
% |
Min. 99 |
Min. 99 |
Min. 99 |
Min. 99 |
IS 1206 |
Penetration @ 25°C (100 grams, 5 seconds) |
0.1 mm |
40-60 |
50-70 |
60-80 |
80-100 |
IS 1203 |
Test on residue from thin film oven tests/RTFOT |
(i) Viscosity ratio @ 60°C |
°C |
Max. 4.0 |
Max. 4.0 |
Max. 4.0 |
Max. 4.0 |
IS 1206 (Part 2) |
(ii) Ductility @ 25°C (Thin film oven test) |
Cm |
Min. 25 |
Min. 40 |
Min. 50 |
Min. 75 |
IS 1208 |
Specification Gravity @ 27/27 |
°C |
Min. 0.99 |
Min. 0.99 |
Min. 0.99 |
Min. 0.99 |
IS 1202 |
Conforms to BIS (IS 73:2006) Specifications |
Dhaduk Petrochemicals Cutback Bitumen Grades Slow Curing (SC) |
Characteristics |
Unit |
SC70 |
SC250 |
SC800 |
SC3000 |
Test Method |
|
Min |
Max |
Min |
Max |
Min |
Max |
Min |
Max |
Kinematic Viscosity @ 60°C |
CST |
70 |
140 |
250 |
500 |
800 |
1600 |
3000 |
6000 |
ASTM D-2170 |
Flash Point |
°C |
66 |
- |
79 |
- |
93 |
- |
107 |
- |
ASTM D-92 |
Penetration @ 25°C, 100 gm, 5 Second |
CM |
40 |
- |
60 |
- |
70 |
- |
80 |
- |
ASTM D-5 |
Distillate, volume percent of total distillate to 360°C |
°C |
10 |
30 |
4 |
20 |
2 |
12 |
- |
5 |
ASTM D-402 |
Ductility @ 25°C, Min |
CM |
100 |
- |
100 |
- |
100 |
- |
100 |
- |
ASTM D-113 |
Solubility in Trichloroethylene, Min |
% |
99 |
- |
99 |
- |
99 |
- |
99 |
- |
ASTM D-2042 |
Water, Max |
%VOL |
- |
0.5 |
- |
0.5 |
- |
0.5 |
- |
0.5 |
ASTM D-95 |
Cutback Bitumen Grades Medium Curing (MC) |
Characteristics |
Unit |
|
|
|
|
|
|
|
|
|
|
Test Method |
MC30 |
MC70 |
MC250 |
MC800 |
MC3000 |
Min |
Max |
Min |
Max |
Min |
Max |
Min |
Max |
Min |
Max |
Kinematic Viscosity @ 60°C |
CST |
30 |
60 |
70 |
140 |
250 |
500 |
800 |
1600 |
3000 |
6000 |
ASTM D-2170 |
Flash Point, Min |
°C |
38 |
- |
38 |
- |
66 |
- |
66 |
- |
66 |
- |
ASTM D-92 |
Penetration @ 25°C, 100 gm, 5 Second |
CM |
120 |
250 |
120 |
250 |
120 |
250 |
120 |
250 |
120 |
250 |
ASTM D-5 |
Distillate Test: Distillate, volume percent of total distillate to 360 °C |
ASTM D-402 |
To 225 °C |
°C |
- |
35 |
- |
25 |
- |
20 |
- |
- |
- |
- |
To 260 °C |
°C |
30 |
75 |
10 |
70 |
5 |
55 |
- |
40 |
- |
15 |
To 316 °C |
°C |
75 |
95 |
65 |
93 |
60 |
90 |
45 |
85 |
15 |
75 |
Residue from distillation to 360 °C, Min |
%VOL |
50 |
- |
55 |
- |
67 |
- |
75 |
- |
80 |
- |
STM D-402 |
Ductility @ 25°C, Min |
CM |
100 |
- |
100 |
- |
100 |
- |
100 |
- |
100 |
- |
ASTM D-113 |
Solubility in Trichloroethylene, Min |
% |
99.0 |
- |
99.0 |
- |
99.0 |
- |
99.0 |
- |
99.0 |
- |
ASTM D-4 |
Water, Max |
%VOL |
- |
0.2 |
- |
0.2 |
- |
0.2 |
- |
0.2 |
- |
0.2 |
ASTM D-95 |
Cut back Bitumen Grades Rapid Curing (RC) |
Characteristics |
Unit |
Specification |
Test Method |
RC 30 |
RC 70 |
RC 250 |
RC 800 |
RC 3000 |
|
|
Min |
Max |
Min |
Max |
Min |
Max |
Min |
Max |
Min |
Max |
|
Kinematic Viscosity @ 60°C |
CST |
30 |
60 |
70 |
140 |
250 |
300 |
800 |
1600 |
3000 |
6000 |
ASTM D-2170 |
Flash Point |
°C |
- |
- |
- |
- |
27 |
- |
27 |
- |
27 |
- |
ASTM D-92 |
Penetration @ 25°C, 100 gm, 5 Second |
CM |
80 |
120 |
80 |
120 |
80 |
120 |
80 |
120 |
80 |
120 |
ASTM D-5 |
Residue from distillation to 360 °C, Min |
ASTM D-402 |
To 225 °C |
°C |
55 |
- |
50 |
- |
35 |
- |
15 |
- |
- |
- |
To 260 °C |
°C |
75 |
- |
70 |
- |
60 |
- |
45 |
- |
25 |
- |
To 316 °C |
°C |
90 |
- |
85 |
- |
80 |
- |
75 |
- |
70 |
- |
Residue from distillation to 360 °C, Min |
%VOL |
50 |
- |
55 |
- |
65 |
- |
75 |
- |
80 |
- |
ASTM D-402 |
Ductility @ 25°C, Min |
CM |
100 |
- |
100 |
- |
100 |
- |
100 |
- |
100 |
- |
ASTM D-113 |
Solubility in Trichloroethylene, Min |
% |
99 |
- |
99 |
- |
99 |
- |
99 |
- |
99 |
- |
ASTM D-2042 |
Water, Max |
%VOL |
- |
0.2 |
- |
0.2 |
- |
0.2 |
- |
0.2 |
- |
0.2 |
ASTM D-95 |
Cut back Bitumen Grades Rapid Curing (RC) |
Dhaduk Petrochemicals Bitumen Emulsion |
Specification of Cationic Bitumen Emulsions |
Quick Setting |
Rapid Setting |
Medium Setting |
Slow Setting |
CQS 1h |
CRS 1 |
CRS 2 |
CMS 2 |
CMS 2h |
CSS 1 |
CSS 1h |
Min |
Max |
Min |
Max |
Min |
Max |
Min |
Max |
Min |
Max |
Min |
Max |
Min |
Max |
Viscosity, Say bolt Furol @ 25°C SFs |
20 |
100 |
- |
- |
- |
- |
- |
- |
- |
- |
20 |
100 |
20 |
100 |
Viscosity, Say bolt Furol @ 25°C SFs |
- |
- |
20 |
100 |
100 |
400 |
50 |
450 |
50 |
450 |
- |
- |
- |
- |
Storage Stability test, 24-h, % A |
- |
1 |
- |
1 |
- |
1 |
- |
1 |
- |
1 |
- |
1 |
- |
1 |
Demulsibility, 35 mL, 0.8 % Dioctyl sodium |
- |
- |
40 |
- |
40 |
- |
- |
- |
- |
- |
- |
- |
- |
- |
Particle charge test |
Positive |
Positive |
Positive |
Positive |
Sieve test, % A |
- |
0.1 |
- |
0.1 |
- |
0.1 |
- |
0.1 |
- |
0.1 |
- |
0.1 |
- |
0.1 |
Cement Mixing test, % |
- |
N/A |
- |
- |
- |
- |
- |
- |
- |
- |
2 |
- |
- |
2 |
Coating ability and water resistance: |
Coating, dry aggregate |
- |
- |
- |
- |
- |
- |
good |
- |
good |
- |
- |
- |
- |
- |
Coating, after spraying |
- |
- |
- |
- |
- |
- |
fair |
- |
fair |
- |
- |
- |
- |
- |
Coating, wet aggregate |
- |
- |
- |
- |
- |
- |
fair |
- |
fair |
- |
- |
- |
- |
- |
Coating, after spraying |
- |
- |
- |
- |
- |
- |
fair |
- |
fair |
- |
- |
- |
- |
- |
Oil Distillate, by volume of emulsion, % |
- |
- |
- |
3 |
- |
3 |
- |
12 |
- |
12 |
- |
- |
- |
- |
Residue % |
57 |
- |
60 |
- |
65 |
- |
65 |
- |
65 |
- |
57 |
- |
57 |
- |
Tests on residue from distillation test: |
Penetration @ 25°C, 100 grams, 5 Second |
40 |
30 |
100 |
250 |
100 |
250 |
100 |
250 |
40 |
90 |
100 |
250 |
40 |
90 |
Ductility, 25°C 5 Cm/Min, Cm |
40 |
- |
40 |
- |
40 |
- |
40 |
- |
40 |
- |
40 |
- |
40 |
- |
Solubility in trichloroethylene, % |
97.5 |
- |
97.5 |
- |
97.5 |
- |
97.5 |
- |
97.5 |
- |
97.5 |
- |